滿足大眾PV3987高光耐磨試驗標準會用到我公司代理的 BYK4563光澤度儀,德國Erichsen249耐磨儀、美國taber5900往復式耐磨試驗機 Rubbing adapter C  刮擦頭
Scrub Resisitance(Micro-Scrach Resistance)of High-Gloss Surfaces in the Vehicle interrior

 

Preface
This satandard supersedes the “Audi AG Provisional Test Specification”and Test Specification PV3975(“Matindale Scrub Resistance”)
Previous issues
PV3987:2016-08
Changes
The folloowing changes have been made to PV3987:2016-08
- section 3.1“Test equipment”:exanple changed
1 Scope
This PV describes a method for testing the micro-Scratch resistance and scrub resistance on high-gloss surfaces
A surface is referres to as high-glossy if the gloss level measurement at an angle of 60° is >70GU。Further gloss level measurements are performed with a measuring angle of 20°
 
This test method is suitable for determining the properties of uncoated (Eg PA PMMA)and coat-ed high-gloss surfaces (eg paint ,in-mold decoration(IMD),in-mold labeling(IML))when they are exposed to low-force friction loads。The load is roughly equivalent to that of the cleaning process the test must be performed on plane surfaces
 
The test determines the relative chang in gloss that is generated by rubbing/Scrubbing with polishing paper on the high-gloss surface
 
2 Designation
Scrub resistance (Micro-scratch resistabce)as per PV3987
 
3 Testing
3.1 Test equipment

Test  equipment Crochmeter as per DIN EN ISO105-X12 or a different testing device with which the required test conditions can be set(testing force 9N,Testing path:104±3mm)
Test  headRubbing adapter C as per DIN55654 (see figure1)
Test equipment/rubbing mediumRolishing paper as per DIN55654:Abrasive grain made of aluminum oxide,semi-open coat density of grain,grain 5um,bonding of grain with full synthetic resin on flexible ,extruded PES film (eg 3M261X)
Cut the polishing paper to an exact width of 25mm and a minimum length of 75mm
Gloss measuring deviceMeasure the gloss level using a reflectometer (as per DIN EN ISO 2813) at angle of 20°

 

3.2 Specimen preparation
A minimum Specimen size of 150mmx100mm is required to perfprm the test
Conditioning
There must be at least 7 days between specimen preparation and testing
For conditioning ,plan for 45h in a standard atmosphere as per VW50554-23/50-2 condition hydrophilic materials(eg polyamides)for 7 days in a standard atmosphere
Specimen preparation
Clean the specimen gently under luder lukewarm running water using only your wet hand
 
A mild laboratory flushing agent that does not leave a greasy residue can be used as a cleaning agent
The surfaces to be tested must not be damaged as a result of cleaning
Then rinse the specimen thoroughly with clear water
Dry the specimen by blowing it off with oil-free compressed air
After cleaning,condition hydrophilic materrials once again for 24h in a standard atmosphere

 

 

3.3 Test procedure
1 condition (see section3.2)
2 clean (see section3.2,for hydrophilic materials ,repeat conditioning if necessary)
3 Meassure the gloss level befor scratching,Measure the gloss level at a measuring angle of 20°
4 Rub/Scratch:Befeor each rubbing process,Clamp in a new rubbing medium。One rubbing
 Process comprise 5 double strokes。Rub with a load of 9N。If the rubbed track is not uniform
(streaky spotted),perform a repeat test
5 After rubbing,store the specimens at room temperature for 24h
6 Measure the gloss level on the track 。Align the gloss measuring device in such a way
 That  themeasuring direction is 90° relative to the rubbing direction。Make sure that the measuring hole of the gloss measuring device rests on the rubbed surface。Do not measure the first and last 10mm of the rubbed track。
 
3.4 Evaluation/assessment
Determine the scrub resistance as a relative change in gloss level(%)with respect to the initial
Gloss level。The measuring angle is 20°
Calculate the relative change in gloss level as follow:
(initial gloss level - gloss level after rubbing)x 100 / initial gloss level

 

4 Applicable documents
The following documents cited in this standard are necessary to its application
Some of the cited documents are translations from the German original。The translations of German terms in such documents may differ from those used in this stand,resulting in terminologocal inconsistency

 

會員登錄

×

請輸入賬號

請輸入密碼

=

請輸驗證碼

收藏該商鋪

X
該信息已收藏!
標簽:
保存成功

(空格分隔,最多3個,單個標簽最多10個字符)

常用:

提示

X
您的留言已提交成功!我們將在第一時間回復您~
撥打電話
在線留言
久久亚洲色一区二区三区| 亚洲国产精品自产在线播放| 日产精品一线二线三线区| 绿帽娇妻在卧室疯狂的呻吟| 中文字幕无码毛片免费看| 三a级做爰片免费观看玉蒲团 | 无码国产精品一区二区免费式影视| 成人精品一区二区三区中文字幕 | 国模生殖欣赏337metcn| 亚洲色无码a片一区二小说| 最近中文2019字幕第二页| 免费 成 人 黄 色 网站69| chinesemature老熟妇高潮| 国产婷婷成人久久av免费高清| 无码人妻久久一区二区三区app| 成人片色情免费观看网站| 精品少妇人妻AV无码久久| 阿娇跪下吃J8图片| 久久久久国色av免费看| 人妻丰满熟妇无码区免费| 国偷自产一区二区免费视频| 午夜欧美精品久久久久久久| 日韩精品无码AV中文无码版| 日韩精品一区二区亚洲AV | 爱的色放在线观看| 亚洲第一综合天堂另类专| 间谍过家家第二季在线观看免费 | 国产人伦人妻精品一区二区| 少妇被粗大猛进去69影院| 琪琪网三级伦锂电影| 亚洲国产精品一区二区久久hs| 国产欧美日韩| 短裙公车被强好爽h吃奶| 久久精品无码av一区二区三区| 精品少妇一区二区三区视频| 国产精品偷窥熟女精品视频| 夹完腿为什么一跳一跳的| 无码熟妇αⅴ人妻又粗又大 | 国产乱码精品一区二区三区久久| 国产精品无码一区二区三区| 国产精品毛片无码|